BÖHLER E110

E110 is a 1.8% Nickel Chromium Molybdenum case hardening steel combining core toughness and high case hardness after carburising and quenching.

Configure & Buy

Technical Data

Chemical Analysis
C Si Mn Ni Cr Mo S P
0.18 0.30 0.50 1.50 1.70 0.30 0.02 0.02
Nearest Standards
AS DIN BS AISI
- 1.6587 / 17CrNiMo6 - -
Heat Treatment
Forge Normalize Anneal Carburize Core Refine Harden Temper Anneal Hardness
850-1150 °C, Cool in furnace. 850-880 °C, Air cool. 650-700 °C, Cool slowly in controlled furnace. 900-950 °C. Furnace or Air cool. 830-870 °C. Oil quench or Air cool. 780-820 °C. Oil quench. 150-200 °C. Air cool. 229 HB max.